Skip to main content Skip to search Skip to main navigation
Izkušnje iz neštetih projektov
Začnimo skupaj
Mi smo drugačni. Mi smo boljši!
Fast and direct contact
Ponuditi
Go to homepage

PQ² Diagram in Die Casting: Matching Machine, Shot End and Gate

PQ² diagram with machine line, die line and operating window beside the shot end of a die casting machine with accumulators
FISS Knowledge · Process

PQ² Diagram in Die Casting: Matching Machine, Shot End and Gate

Clamping force and shot weight show whether a die fits onto a machine. Whether the shot end can push the metal through the gates fast enough is a question of hydraulic power against flow resistance – answered by the PQ² diagram.

Short Answer

What Is a PQ² Diagram in Die Casting?

A PQ² diagram plots metal pressure P against the square of the flow rate Q. On these axes, the performance of the shot end (machine line) and the flow resistance of the die and its gates (die line) both become straight lines, so their intersection shows the highest flow rate this machine can drive through this die.

Limits for fill time and gate velocity add the operating window. A PQ2 diagram in die casting thus shows before the first shot whether machine, plunger and gate area fit together.

Machine Line

How Is the Machine Line Drawn?

The machine line describes what the shot end can deliver. NADCA course material draws it as a straight line from the static metal pressure at zero flow to the maximum flow rate at zero pressure. The effective shot cylinder pressure falls with the square of plunger velocity, p = p(hydraulic) · (1 − (v / v(dry shot))²), so the line is straight on P–Q² axes.

  • Static metal pressure: pm = p(hydraulic) · (d(shot cylinder) / d(plunger))² – hydraulic pressure transmitted through the plunger at rest.
  • Maximum flow rate: Qmax = A(plunger) · v(dry shot), with A = π · d² / 4.
  • Dry shot speed: plunger velocity with the shot valve fully open and an empty sleeve. Per NADCA it is unique to each machine, changes with wear and should be measured and documented.
Shot Valve

Throttling the Flow

Less flow, unchanged static pressure.

Accumulator

Lower Charge Pressure

Static pressure and maximum flow both fall.

Plunger

Smaller or Larger Diameter

Smaller: more pressure, less flow; larger: the reverse.

Die Line

What Determines the Die Line: Gate Area and Discharge Coefficient

The die line shows the pressure the metal needs to pass the gates at a given flow rate. From Bernoulli: p = ρ / 2 · (v(gate) / Cd)², with v(gate) = Q / A(gate). For a fixed gate area the die line starts at the origin; a smaller gate makes it steeper, a larger gate flatter.

The discharge coefficient Cd lumps friction, deflection and contraction losses into one number below 1. The NADCA course material gives typical values of 0.5 to 0.6 for aluminium and 0.6 to 0.7 for zinc and magnesium; the Altair Inspire Cast documentation states roughly 0.5 to 0.7 depending on material.

Calibrate Cd on Real Jobs Cd is empirical, not a material constant. The NADCA material recommends determining it from jobs that run successfully – far more reliable than a textbook value.
Operating Window

Which Limits Define the PQ² Operating Window?

Four lines bound the operating window: two vertical (flow rate) and two horizontal (gate pressure from the minimum and maximum gate velocity, via Bernoulli).

Boundary Derived From Risk Outside the Boundary Values Found in the Sources
Minimum flow rate Maximum fill time (volume / time) Cold shuts, misruns, poor surface 0.03–0.3 s, mostly 0.03–0.1 s (Torino thesis)
Maximum flow rate Machine line meets die line Not achievable Machine-specific
Minimum gate velocity Atomised flow at the gate Coarse flow, entrapped air Aluminium 600–1600 in/s ≈ 15–41 m/s (NADCA)
Maximum gate velocity Die erosion and soldering Erosion, solder, pressure spikes Generally 20–60 m/s (Torino thesis)

The maximum fill time is usually estimated with the NADCA gating equation t = k · ((Ti − Tf + S · Z) / (Tf − Td)) · T (wall thickness T, temperatures, permitted solid fraction S, alloy constants k and Z). Why speed alone does not guarantee quality is explained in Mold Filling and Vacuum in Die Casting; the erosion side is covered in Die Life: Heat Checking, Soldering and Erosion.

Worked Example

Worked Example: One Die, Three Shot End Set-ups

Illustrative figures, only showing the method. Die: 3.0 kg aluminium through the gates at 2.4 g/cm³ = 1,250 cm³; maximum fill time 50 ms, so at least 25 L/s; gate area 800 mm²; Cd 0.5; gate velocity window 20–40 m/s. At 25 L/s: about 31 m/s and 47 bar at the gate.

Set-up Static Metal Pressure Qmax (Dry Shot) Max. Flow Through This Die Shortest Fill Time
A: 140 bar, shot cylinder Ø 200 mm, plunger Ø 80 mm, dry shot 6 m/s ≈ 875 bar ≈ 30 L/s ≈ 29 L/s ≈ 43 ms
A with plunger Ø 90 mm ≈ 691 bar ≈ 38 L/s ≈ 36 L/s ≈ 35 ms
B: 160 bar, shot cylinder Ø 180 mm, plunger Ø 80 mm, dry shot 8 m/s ≈ 810 bar ≈ 40 L/s ≈ 38 L/s ≈ 33 ms

The 40 m/s limit caps useful flow at 32 L/s, so the window spans 25–32 L/s. Set-up A covers only part of it, with little reserve if the dry shot speed drops. The 90 mm plunger covers it at lower static pressure and a lower sleeve fill ratio – see Shot Weight and Casting Volume. Set-up B covers it with the original plunger.

Used Machines

How Do You Compare a Used Shot End With a Die?

For a used cold-chamber machine, the PQ² diagram turns a data sheet comparison into a check against a real die (practical outline, not a manufacturer procedure).

01

Collect Die Data

Volume through the gates, gate area, wall thickness, alloy, proven fill time.

02

Measure the Machine

Shot pressure, cylinder diameter, available plungers and a measured dry shot speed, not the brochure value.

03

Draw Both Lines

One machine line per plunger, the die line and the window.

04

Check the Reserve

The intersection should lie clearly beyond the required flow rate.

05

Confirm With Shot Curves

Compare trial shot data with the calculated operating point.

Reading the traces is covered in Understanding Shot Curves. A low dry shot speed often points to accumulators or valves – see Hydraulics of Die Casting Machines. More checks: Buying a Used Die Casting Machine.

Limitations

What the PQ² Diagram Cannot Show

The PQ² diagram is a steady-state energy balance – fast and transparent, but limited:

  • Plunger acceleration and braking are ignored; the fill rate is assumed constant.
  • Runner losses and gate geometry are lumped into Cd.
  • Slow phase and air in the shot sleeve are not covered.
  • Intensification is a separate system.
  • Flow patterns, venting and solidification stay invisible.

For these questions, simulation is the next step – see Die Casting Simulation.

Conclusion

Machine Line, Die Line, Window: The PQ² Check in Brief

The PQ² diagram connects shot end hydraulics, plunger size and gate design. With a measured dry shot speed, a realistic discharge coefficient and sourced limits for fill time and gate velocity, it shows quickly whether a machine fills a die with reserve – and whether another plunger or gate area widens the window.

Frequently Asked Questions

Questions About the PQ² Diagram

Why Is Q Squared in the PQ² Diagram?

Gate pressure loss and the pressure drop in the shot system both rise with the square of flow rate. Plotting P against Q² turns both curves into straight lines drawn from two points each.

Where Does the Dry Shot Speed Come From?

The dry shot speed is measured on the machine: shot valve fully open, empty sleeve, production hydraulic pressure. Because it changes with wear, a measured value beats a brochure figure.

What Happens if the Operating Point Lies Outside the Window?

Left of the window, fill times are too long and cold shuts become likely. Above it, gate velocity drives erosion and soldering. If no window point lies below the machine line, gate area, plunger or machine must change.

Does the PQ² Diagram Replace Simulation?

No. The PQ² diagram checks whether pressure and flow rate fit, but shows no flow fronts, air entrapment or solidification. Simulation and trial shots confirm the result.

Checking a Shot End?

Compare Used Die Casting Machines With Your Die.

FISS lists used cold-chamber die casting machines. Send us your die data and machine requirements, and we will discuss which shot end data to check.

Sources

NADCA / M. Ward: PQ² – course presentation (EC-700 Alucast), North American Die Casting Association, November 2013.

North American Die Casting Association (NADCA): Determine Optimally Sized Gates While Taking into Consideration PQ² Analysis, webinar series description, 2023, accessed 19 November 2026.

G. Lanzoni: Simulation and validation of high-pressure die casting of an electric motor housing for automotive application, master’s thesis, Politecnico di Torino, 2020/2021, accessed 19 November 2026.

Altair: Inspire Cast – High Pressure Process, online help 2023, accessed 19 November 2026.

FISS Machines: Shot Weight and Casting Volume and Mold Filling and Vacuum in Die Casting, fiss-machines.com, accessed 19 November 2026.